Polyarylate resin

UNIFINER

General Properties of UNIFINER

  Properties Measurement
condition
Standards
JIS
Unit M-2000H
Ultra Heat
Resistance
M-2040
Easy
Solubility
M-2040H
Easy
Solubility
U-100
U-Polymer
Thermal Glass transition temperature — K 7121 °C 275 220 235 193
Thermal conductivity — — W/m·K — — — 0.14
Coefficient of linear thermal
expansion
— K 7197
basis
10-6/°C 70 80 80 88
Specific heat — K 7123 J/g·K — — — 1.17
Physical Density — K 7112 g/cm³ 1.12 1.17 1.17 1.21
Water absorption (immersion) 23°C/24h K 7209 % 0.3 0.4 0.4 0.5
Tensile strength at yield — K 7127 MPa 71 72 73 65
Tensile elongation at break — K 7127 % 30 18 66 60
Tensile modulus — K 7127 MPa 1900 1900 1900 1840
Surface hardness Pencil hardness K 5600-5 — HB 2B — HB
Optical Light transmittance — K 7361-1 % 89 89 89 89
Refractive index — K 7142 — 1.58 1.60 1.60 1.61
Photoelastic coefficient — — cm²/dyn — — — 130×10-12
Electrical Dielectric breakdown strength — K 6911 kV/mm 110 120 126 160
Surface resistivity — K 6911 Ω More than
1014
More than
1014
More than
1014
More than
1014
Volume resistivity — K 6911 Ω·cm More than
1014
More than
1014
More than
1014
More than
1014
Dielectric constant
(Dk, ε)
60Hz C 6481 — 2.9 3.2 3.2 3.2
1kHz 2.9 3.2 3.2 3.2
1MHz 2.8 3.1 3.1 3.2
1GHz Cavity resonance
method
2.6 2.7 2.7 2.8
5GHz 2.6 2.6 2.6 2.8
10GHz 2.6 — — —
Dissipation factor
(Df, tanδ)
60Hz C 6481 — 0.002 0.003 0.003 0.002
1kHz 0.003 0.003 0.003 0.003
1MHz 0.02 0.02 0.02 0.02
1GHz Cavity resonance
method
0.008 0.007 0.007 0.007
5GHz 0.006 0.005 0.005 0.006
10GHz 0.006 — — —

* Measurement Thickness : 100µm